- 密度 [g/cm3]: 2.18
- 弯曲强度 [MPa]: 35.0
Physical Properties | Metric | English | Comments |
---|---|---|---|
Density | 2.18 g/cc | 0.0788 lb/in³ | ASTM D792 |
Apparent Bulk Density | 0.360 g/cc | 0.0130 lb/in³ | ASTM D4894 |
Water Absorption | 0.00 % | 0.00 % | ASTM D570 |
Linear Mold Shrinkage | 0.039 cm/cm | 0.039 in/in | Radial shrinkage of 10 cm o.d. sintered rod at 23°C |
Mechanical Properties | Metric | English | Comments |
Tensile Strength, Ultimate | 35.0 MPa | 5080 psi | ASTM D638 |
Elongation at Break | 500 % | 500 % | ASTM D638 |
Coefficient of Friction, Dynamic | 0.060 | 0.060 | ASTM D1894 |
Coefficient of Friction, Static | 0.080 | 0.080 | ASTM D1894 |
Electrical Properties | Metric | English | Comments |
Electrical Resistivity | 1.00e+18 ohm-cm | 1.00e+18 ohm-cm | ASTM D257 |
Dielectric Constant | 2.1 @Frequency 60.0 - 2.00e+9 Hz | 2.1 @Frequency 60.0 - 2.00e+9 Hz | ASTM D150 |
Dielectric Strength | 100 kV/mm | 2540 kV/in | ASTM D149 |
Dissipation Factor | >= 0.00030 @Frequency 60.0 - 2.00e+9 Hz | >= 0.00030 @Frequency 60.0 - 2.00e+9 Hz | ASTM D150 |
Thermal Properties | Metric | English | Comments |
Thermal Conductivity | 0.240 W/m-K | 1.67 BTU-in/hr-ft²-°F | ASTM C177 |
Maximum Service Temperature, Air | 260 °C | 500 °F | Continuous Service |
Flammability, UL94 | V-0 | V-0 | VE-0 |
Oxygen Index | >= 95 % | >= 95 % | ASTM D2863 |