- 密度 [g/cm3]: 1.49
 
| Physical Properties | Metric | English | Comments | ||
|---|---|---|---|---|---|
| Density | 1.49 g/cc | 0.0538 lb/in³ | (DAM); ISO 1183 | ||
| Moisture Absorption at Equilibrium | 1.7 % | 1.7 % | Humidity Absorption (DAM); Sim. to ISO 62 | ||
| Mechanical Properties | Metric | English | Comments | ||
| Tensile Strength at Break | 67.0 MPa | 9720 psi | ISO 527-1/-2 | ||
| Elongation at Break | 6.0 % | 6.0 % | ISO 527-1/-2 | ||
| Tensile Modulus | 4.80 GPa | 696 ksi | ISO 527-1/-2 | ||
| Charpy Impact, Notched | 0.300 J/cm² @Temperature -30.0 °C  | 1.43 ft-lb/in² @Temperature -22.0 °F  | ISO 179/1eA | ||
| 0.600 J/cm² @Temperature 23.0 °C  | 2.86 ft-lb/in² @Temperature 73.4 °F  | ISO 179/1eA | |||
| Electrical Properties | Metric | English | Comments | ||
| Volume Resistivity | 1.00e+12 ohm-cm | 1.00e+12 ohm-cm | IEC 60093 | ||
| Surface Resistance | 1.00e+13 ohm | 1.00e+13 ohm | IEC 60093 | ||
| Dielectric Constant | 4.5 @Frequency 1e+6 Hz  | 4.5 @Frequency 1e+6 Hz  | IEC 60250 | ||
| 14 @Frequency 100 Hz  | 14 @Frequency 100 Hz  | IEC 60250 | |||
| Dielectric Strength | 30.0 kV/mm | 762 kV/in | IEC 60243-1 | ||
| Dissipation Factor | 0.12 @Frequency 1e+6 Hz  | 0.12 @Frequency 1e+6 Hz  | IEC 60250 | ||
| 0.32 @Frequency 100 Hz  | 0.32 @Frequency 100 Hz  | IEC 60250 | |||
| Thermal Properties | Metric | English | Comments | ||
| Melting Point | 220 °C | 428 °F | 10°C/min (DAM); ISO 11357-1/-3 | ||
| Descriptive Properties | |||||
| Heat stabilized or stable to heat | Yes | ||||
| Injection Molding | Yes | ||||
| Lubricants | Yes | ||||
| Release agent | Yes | ||||
| With fillers | Yes | ||||